AGAR Structure
Harzlas AGAR is a series of thin-film layers coated on plastic substrates. Typically, it consists of a hard coat layer, AR layers with AG surface treatment, and an anti-fingerprint layer. We can customize the layers to meet the requirements for your project.
- Developed specially for in-vehicle use such as for car navigation systems
- Excellent resistance to UV degradation and common household chemicals
- The anti-reflective coating is applied to follow the shape of the surface of the substrate, resulting in an evenly applied coating
- The haze of the substrate can be adjusted to approximately 1-15%. Other options may be available upon consultation
Properties
Low Reflectance
Reduce the amount of light that gets reflected to the user.
High Transmittance
Improved clarity allows you to see the other side without hindrance.
High Chemical Resistance
Cleanable with common household chemicals without worrying about deteriorating the coating.
Water and Oil Repellent
Easy clean smudges and fingerprints with our specially formulated anti-fingerprint coating.
High Durability
Excellent scratch and abrasion resistance for long lasting usability.
Consistent Reflected Color
Our highly controlled production process allows for the coating to be evenly applied at the nanometer level, resulting in a consistent reflection color throughout the substrate.
Environmental Resistance Tests
Test | Conditions | Result |
---|---|---|
High Temperature | 100C for 192 hours | No Deterioration in Optical Properties or Adhesion |
Low Temperature | -40C for 192 hours | No Deterioration in Optical Properties or Adhesion |
Thermal Shock | -40C to 95C, 200 cycles, 30 minutes per temperature | No Deterioration in Optical Properties or Adhesion |
High Heat and Humidity | 65C, 95%RH, 192 hours | No Deterioration in Optical Properties or Adhesion |
Chemical Resistance Tests
Test | Conditions | Result |
---|---|---|
Tap Water | 25C, 96 hours | No Deterioration in Adhesion |
5% Saline Solution | 25C, 96 hours | No Deterioration in Adhesion |
Acidic Artificial Sweat | 25C, 96 hours | No Deterioration in Adhesion |
Alkaline Artificial Sweat | 25C, 96 hours | No Deterioration in Adhesion |